Abstract
The datasets presented here are related to the research paper entitled "Disordered Gd(6)UO(12-δ) with the cation antisite defects prepared by a combined mechanochemical-thermal method"[1]. The datasets complement the findings [1] on the effect of the combined mechanochemical-thermal processing of the stoichiometric mixture of solid precursors (3Gd(2)O(3) + UO(2)) on the formation of Gd(6)UO(12-δ) phase. In this article, we provide (i) X-ray diffraction (XRD) data of the 3Gd(2)O(3) + UO(2) mixture milled for 12 h, (ii) the refined XRD data of the non-milled 3Gd(2)O(3) + UO(2) mixture after annealing at 1282 °C for 3 h in air, and (iii) the thermogravimetric and differential thermal analysis (TG-DTA) data for non-milled and mechanically preactivated 3Gd(2)O(3) + UO(2) mixture measured in air at a heat rate of 10 K/min.